Optimization of Shrinkage and Axial Distortion in an Investment Casting CF8M Assembly Cover
Improving Cavity Shrinkage and Structural Deformation From Reducing The Internal Stress Buildup to Optimizing Mold Flow
Our customers often require precision-cast stainless steel (CF8M) parts with significant shape variations and prone to deformation. During production, we frequently encounter quality issues, including shrinkage cavities in corners and surface deformation. Leveraging its extensive experience in stainless steel precision casting, Teamco optimized the casting process by adjusting material properties, casting temperature, solidification sequence, and pouring conditions, as well as process control parameters. This eliminated the need for new molds unless absolutely necessary, successfully eliminating major casting defects and stabilizing critical dimensions. The optimized mass-produced parts exhibited consistent quality and maintained the original design as required by the customer.
This case demonstrates Teamco's ability to solve casting problems using engineering expertise, process optimization, and extensive practical experience. By minimizing additional costs, we consistently provides clients with high-quality products and timely delivery. Teamco offers more than just quality improvements for individual products, we focus on providing long-term solutions that ensure smooth mass production for every product our customer desires.
| Case: | Optimization of Shrinkage and Axial Distortion in an Investment Casting CF8M Assembly Cover |
|---|---|
| Customer Country: | Germany |
| Application: | Heavy-Duty Locking Components |
| Product Name: | Locking Cover |
| Production: | Investment Casting (Lost-Wax Casting) |
Customer Requirement
Material Specification: CF8M (316 Austenitic Stainless Steel) casting.
Component Type: Assembly cover has an L junction corner with wall thickness 6mm and 2mm respectively; besides, this area contains a cast assembly pillar featuring an outer diameter Ø5mm with a a height of 9mm.
Geometric Constraints: A severe wall thickness transition at this L conjunction corner, dropping from 6 mm to 2mm—a 3:1 ratio, posing a shrinkage risk at the corner end. Additionally, the small assembly pillar has a high ratio of height-to-outer-diameter, raising concerns about deformation, yet the customer is not considering any design changes.
Production Volume: Small-to-medium batch production of 1,000 to 2,000 pieces per annum.
Technical Issues or Challenges
This component has two main defects: shrinkage cavities at the casting corners and an axial deformation exceeding the standard by 0.3mm on the Ø5mm assembly column, affecting customer assembly.
- CF8M has low thermal conductivity and high linear shrinkage: During molten metal casting, the thicker 6mm T-shaped corner stores more heat, while the adjacent 2mm thinner wall solidifies prematurely before the molten metal has flowed through the complete runner, resulting in incomplete casting and isolation from the hot spot of the T-shaped molten metal, causing localized shrinkage.
- During solidification, the thin-walled portion shrinks first and is subjected to unilateral tensile force: The portion that shrinks first has higher strength and constrains the direction of subsequent shrinkage, thus generating stress. When the stress exceeds the limit, deformation occurs.
Teamco Solutions
Given the annual volume of 1,000–2,000 pieces, investment in modifying the tooling is not economical. Therefore we implemented a high-efficiency engineering matrix combining mechanical restraint, enhanced localized heat dissipation, and refined thermal parameters without altering the customer's design footprint.
1. Mechanical Restraint: Temporary Anti-Distortion Tie Bars
Action: integrated a temporary small size wax tie bar manually bridging the Ø5 mm pillar core to the thin-wall rim.
Metallurgical Principle: This solidifies in sync with the thin wall, also establishes a structural lock with the thick wall. This counteracts the unilateral thermal pull and holds the pillar’s axis within tolerance.
2. Optimize Corner Fillets
Measures: Adjust corner fillets appropriately during mold opening. For areas with abrupt changes in wall thickness, use bevels or fillets to connect them, avoiding shrinkage cavities.
Principle: Fillets that are too large or too small can lead to difficulties in compensating for shrinkage or problems with cooling. Appropriate adjustments can effectively prevent these problems.
3. Thermal Process Refinement
Action: Lowered the pouring temperature extended the in-mold dwell time before knockout.
Metallurgical Principle: Minimizing superheat reduces the total liquid contraction at the hot spot. Prolonged slow-cooling within the insulating shell ensures that residual macro-stresses are uniformly relieved, preventing post-solidification warpage.
Results and Customer Benefit
| Items | Problem Types | After Optimization | Benefits |
|---|---|---|---|
| Shrinkage | Unpredictable voids at inner corner after sandblasting | Obviously improved, no abnormality | Meet quality standards |
| Axial Alignment | Pilar axial out of spec. deviation >0.3 mm | Effectively controlled to within tolerance | 100% Assembly Pass Rate |
| Tooling Re-engineering Cost | High | $0 (Zero modification to tooling die) | Maintain customer’s original design |
| Production Yield | Impact rate >20% due to scrap/rework | Achieved stable yield | Brought to on-time delivery |
Through this precision casting solution optimization focused on key improvements, the customer obtained CF8M assembly cover parts with dimensions perfectly matching their requirements. These parts could be smoothly assembled on the production line, achieving perfect compliance without the need for costly product design changes or reinvestment in mold capital. Teamco continues to solve customers’ problems with professionalism and technology, allowing customers to confidently entrust their castings to us for production.